Experimental Results


Experiment 1

Conditions: Charge of 1.0g of biotite mica, passed through 400 μm aperture sieve; 10 ml of propan-2-ol. Ground for 10 minutes with corundum grinding pellets.

Result:1.0g of dried product recovered. Average diameter of product was 5 μm, Largest particle present was 10 μm.


Experimental Results

 

Experiment 2

Conditions:Charge of 2.0g of graded Belgian optical glass silica sand of particle size 285 μm ± 15 μm; 10 ml of water. Ground for 10 minutes with corundum grinding pellets

Result: 2.0g of dried product recovered. Average diameter of product was 6 μm. Largest particle size was 14 μm.

  